DrawingToolChip

Machining 1045 and 4140 Carbon and Alloy Steel

The hardness and condition on the bar certificate set the speed, depth of cut and power for 1045 and 4140, so put the range on the order.

CNC machined steel parts, a 1045 carbon steel shaft with a keyway and a 4140 alloy steel gear blank with a black oxide finish.

In 1931 the National Bureau of Standards turned forgings dry with high-speed steel tools at a feed of 0.29 mm (0.0115 in.) per revolution and a depth of cut of only 0.25 mm (0.010 in.). With those shallow cuts the plain 0.4 % carbon steel was, apart from one annealed nickel-chromium grade, the hardest of the group to machine and gave the poorest finish, while chromium with molybdenum was the most effective alloy combination near 620 MPa (90,000 psi). The same report warned that the ranking changed with heavier roughing cuts. Nearly a century later the lesson still holds for 1045 and 4140: which steel cuts better depends on its hardness and on the depth of cut, not on the name.

How 1045 and 4140 Differ Before the First Cut

The two grades share a carbon level and little else. FM Carbide’s technical reference gives 1045 as a plain medium-carbon steel of 0.43 to 0.50 % carbon and 0.60 to 0.90 % manganese, with phosphorus at 0.04 % and sulfur at 0.05 % maximum, and no deliberate chromium, molybdenum or nickel. Its 4140 page gives 0.38 to 0.43 % carbon, 0.75 to 1.00 % manganese, 0.80 to 1.10 % chromium and 0.15 to 0.25 % molybdenum.

Table 1. Composition and equivalent designations of 1045 and 4140, as listed by a cutting tool maker’s material reference.
Item 1045 4140
Steel family plain medium-carbon chromium-molybdenum low alloy
Carbon, % 0.43 to 0.50 0.38 to 0.43
Manganese, % 0.60 to 0.90 0.75 to 1.00
Chromium, % not added 0.80 to 1.10
Molybdenum, % not added 0.15 to 0.25
EN and DIN C45, 1.0503 42CrMo4, 1.7225
JIS S45C SCM440(H)
BS 080M46 708M40
Typical supply, per the same reference as rolled or normalized, or hardened and tempered most often pre-hardened and tempered

The supply condition matters more than the chemistry for the cutting room. The same reference describes 4140 in the annealed state as machining like a mid-carbon steel, and in the pre-hardened state as raising cutting forces, heat at the tool-chip interface and flank wear, because its chromium and molybdenum form fine abrasive carbides. 1045 carries no such carbides, so its abrasive wear stays lower than that of alloy grades at similar hardness.

Cutting Tool Engineering’s guide to turning carbon steels sets 1045 inside the medium-carbon group, AISI 1029 to 1053, with 0.25 to 0.55 % carbon and 0.30 to 1.00 % manganese. It also notes that the turning test used to rate the tool life of indexable insert grades runs on AISI 1045 as the standard workpiece.

1045 and 4140 arrive at the machine as conditions, not as names. The hardness on the certificate decides the cutting data more than the second digit of the grade.

Hardness Sets the Cutting Speed for Both Grades

Tool makers sort steels into groups by carbon, alloy and hardness, and the group sets the starting speed. Haas Automation’s speeds and feeds sheet for its turning inserts puts medium- and high-carbon steels above 0.3 % carbon in group P2, alloy steels below 330 HB (35 HRC) in P3, and alloy steels at 340 to 450 HB (36 to 48 HRC) in P4. Annealed or lightly tempered 4140 falls in P3, and through-hardened 4140 in P4.

Table 2. Starting turning speeds for two coated carbide grades by material group, from Haas Automation’s turning insert sheet.
Material group Hardness Grade HTP15, m/min (ft/min) Grade HTP25, m/min (ft/min) Applies to
P2, medium- and high-carbon steel over 0.3 % C not stated 265 (870) 195 (640) 1045
P3, alloy steel below 330 HB (below 35 HRC) 190 (625) 155 (510) 4140 annealed or tempered below 330 HB
P4, alloy steel 340 to 450 HB (36 to 48 HRC) 145 (475) 105 (345) 4140 through-hardened

The step from P3 to P4 cuts the starting speed of the same insert grade by about a quarter to a third. A part ordered in 4140 at 28 to 32 HRC and a part ordered at 40 to 44 HRC are therefore two different machining jobs, even on the same drawing.

Two Tool Makers, Two Starting Points

Starting values differ between makers, and the conditions behind them are not always printed. FM Carbide lists 1045 at 240 to 330 m/min (790 to 1,080 ft/min) for turning, 150 to 205 m/min (490 to 670 ft/min) for milling, 115 to 155 m/min (380 to 510 ft/min) for parting, 135 to 185 m/min (440 to 610 ft/min) for grooving and 95 to 130 m/min (310 to 430 ft/min) for drilling. For 4140 it lists turning at 260 to 355 m/min (850 to 1,160 ft/min) and milling at 160 to 220 m/min (520 to 720 ft/min), without a hardness beside the figures.

Those 4140 values sit above the 1045 values from the same source, which only makes sense for annealed stock. The maker qualifies all its figures as favorable conditions: a matched grade, rigid clamping, short overhang, good stock and nominal hardness, to be lowered for interrupted cuts, weak setups or harder material. For a solid carbide end mill in 4140, RobbJack’s tested starting points use a four-flute AlTiN-coated tool at 122 m/min (400 ft/min), with a chip load rising from 0.008 mm (0.0003 in.) per tooth at 3.2 mm (1/8 in.) diameter to 0.051 mm (0.0020 in.) at 12.7 mm (1/2 in.).

A buyer comparing quotations does not need to choose between these numbers. What matters is that the hardness range is on the order, because every one of these tables changes row when it moves.

Depth of Cut and Feed in Roughing, Semifinishing and Finishing

Depth of cut is where the three passes of a turned 1045 part separate. Cutting Tool Engineering’s Table 3 for medium-carbon steels, adopted from the Machining Data Handbook, gives one set of conditions per pass and per hardness band, with coated carbide grades CP30 for roughing, CP20 for semifinishing and CP10 for finishing.

Table 3. Turning conditions for medium-carbon steels such as 1045, by hardness and pass, from Cutting Tool Engineering’s guide, Table 3.
Hardness, HB Pass Depth of cut, mm (in.) Feed, mm/rev (in./rev) Cutting speed, m/min (ft/min) Coated carbide, ISO
125 to 175 roughing 7.6 (0.300) 0.51 (0.020) 145 (475) CP30
125 to 175 semifinishing 3.8 (0.150) 0.38 (0.015) 183 (600) CP20
125 to 175 finishing 1.0 (0.040) 0.18 (0.007) 282 (925) CP10
175 to 225 roughing 7.6 (0.300) 0.51 (0.020) 126 (415) CP30
175 to 225 semifinishing 3.8 (0.150) 0.38 (0.015) 160 (525) CP20
175 to 225 finishing 1.0 (0.040) 0.18 (0.007) 239 (785) CP10
225 to 275 roughing 7.6 (0.300) 0.51 (0.020) 122 (400) CP30
225 to 275 semifinishing 3.8 (0.150) 0.38 (0.015) 152 (500) CP20
225 to 275 finishing 1.0 (0.040) 0.18 (0.007) 229 (750) CP10

The table reads in two directions. Down each hardness band, a lighter cut and a finer feed allow a faster speed; across the bands, every pass slows as hardness rises. The finishing speed at 225 to 275 HB is about 19 % below the finishing speed at 125 to 175 HB.

Holding the Removal Rate When the Depth Changes

The same guide gives a rule for conditions that fall between the rows: change the speed so that the metal removal rate stays where the table puts it. Its worked case starts from 168 m/min (550 ft/min), a 7.62 mm (0.300 in.) depth and a 0.51 mm (0.020 in.) feed, which removes 649 cm³ (39.6 in.³) per minute. Cutting the depth to 5.08 mm (0.200 in.) while keeping the removal rate calls for 251 m/min (825 ft/min), the speed raised in proportion to the depth lost.

The same rule works for any pair of rows: the product of speed, depth and feed is held, so whatever is taken from one is given back to another.

Chipbreaker Windows

An insert’s chipbreaker sets the depth and feed it can control. Haas prints a window for each of its turning chipbreakers on log axes of depth of cut against feed. Read from those charts, the finishing breaker HFF covers depths from about 0.3 mm up to between 2 and 4 mm (about 0.01 to 0.12 in.) at feeds below about 0.4 mm per revolution, while the roughing breaker HMR, described as an excellent choice for steels and difficult materials, reaches past 8 mm (0.31 in.) of depth. The values are approximate, read from the drawn windows rather than from printed numbers.

A finishing pass of 1.0 mm (0.040 in.), as in Table 3, sits inside a finishing window. A roughing pass of 7.6 mm (0.300 in.) needs a roughing breaker, and a last pass lighter than the lowest depth of a window leaves the breaker outside the range its maker drew for it.

Shallow Cuts, Roughing Cuts and the Ranking of the Two Steels

The 1931 study by T. G. Digges at the Bureau of Standards remains one of the few open comparisons of a plain carbon steel and a chromium-molybdenum steel at matched strength. The forgings were heat treated to tensile strengths between about 517 and 1,517 MPa (75,000 and 220,000 psi), and the tests used shallow cuts, with tool failure taken at 0.025 to 0.05 mm (0.001 to 0.002 in.) of wear.

Its conclusions bear directly on 1045 and 4140.

  1. Machinability was measured as the cutting speed that gives a set tool life, and measurable, consistent differences appeared between the steels.
  2. A steel that allows a higher speed at one tensile strength does not necessarily keep its lead at another strength.
  3. The 0.4 % plain carbon steel, SAE 1040, was the most difficult to machine with shallow cuts apart from an annealed nickel-chromium steel, and gave poorer finishes than the alloy steels.
  4. One heat treatment of the carbon steel, leaving partially spheroidized cementite, gave a medium smooth and satisfactory finish and the best machinability of the carbon steel group.
  5. Chromium and molybdenum were the most effective combination at the lower strengths, about 620 MPa (90,000 psi), and nickel with chromium or chromium with vanadium near 1,240 MPa (180,000 psi).
  6. Steels that machined well with shallow cuts did not necessarily machine well with roughing cuts.

The report ties the advantage of the alloy steels to the combined effect of all their elements, carbon included, rather than to any one addition. For a modern buyer the practical reading is narrower. The finish on a 1045 part depends heavily on its microstructure, and the same grade can finish poorly in one heat treatment and satisfactorily in another, as the partially spheroidized bar did in the 1931 tests.

A ranking of 1045 against 4140 holds only at one hardness and one depth of cut. Change either and the order can reverse.

Cutting Force and Spindle Power at Higher Hardness

Harder steel needs more power for the same chip. NASA’s report SP-5084 on machining ultrahigh-strength steels, prepared by Battelle for the Marshall Space Flight Center, puts the unit power for low-alloy steels heat treated to 350 HB at roughly 0.055 to 0.068 kW per cm³ per minute (1.2 to 1.5 hp per in.³ per minute), against about 0.036 kW (0.8 hp) for carbon steels.

A worked example shows what the difference does to a machine. Roughing at 150 m/min (492 ft/min), 3 mm (0.118 in.) deep and 0.3 mm (0.012 in.) per revolution removes 135 cm³ (8.2 in.³) per minute.

  • In a carbon steel at about 0.036 kW per cm³ per minute, that pass needs about 4.9 kW (6.6 hp) at the cutting edge.
  • In a low-alloy steel at 350 HB, at 0.055 to 0.068 kW per cm³ per minute, the same pass needs about 7.4 to 9.2 kW (9.9 to 12.3 hp).

The report also lists machinability ratings against B1112 steel at 100. Cold drawn 1020 rates 70, annealed and cold drawn 4130 rates 70, and the same 4130 quenched and tempered to 350 HB rates 30. 4140 is not in the table, but its chromium-molybdenum neighbor shows how far a hardened alloy part falls from its annealed rating.

The same document describes a sequence used on critical parts: machining near 350 HB to almost final size, then heat treating to about 500 HB and finishing by machining or grinding. For 4140 parts with a high final hardness, that split keeps most of the metal removal in the softer condition, where Table 2 gives the faster rows.

Edge Preparation and Rubbing

FM Carbide’s reference recommends, for 1045, a hone of 0.05 to 0.08 mm (0.002 to 0.003 in.), a rake angle of 11 to 13° and a positive land 0.20 to 0.30 mm (0.008 to 0.012 in.) wide. For both grades it treats work hardening as a modest concern: light cuts, dull edges or dwelling can harden the surface locally and make the next pass harder, far less than on austenitic stainless steel. Its advice for 4140 is rigid setups, positive rake and steady feeds that keep the tool cutting rather than rubbing.

Ordering Bar for a Machined 1045 or 4140 Part

The cutting data above turns on facts that only the order can supply. Without them a supplier quotes against an assumed condition and discovers the real one at the first cut.

  • Grade and standard, for example AISI 1045 or C45 (1.0503), AISI 4140 or 42CrMo4 (1.7225), named as the drawing intends.
  • Condition, such as as-rolled, normalized, annealed, or hardened and tempered.
  • Hardness range on the delivered bar, in HB or HRC, since it moves the job between the P2, P3 and P4 groups.
  • Heat treatment after machining, if any, with the final hardness, so that roughing and finishing allowances are planned.
  • Surface finish on functional faces, since finish on plain carbon steel depends on microstructure as much as on the tool.

A part that moves from a handful of pieces to a steady run usually keeps its grade but can change its condition, for example from bar machined after hardening to bar roughed soft and finished hard. A buyer planning that move can read about low-volume metal CNC and bridge production with the condition and hardness range already fixed on the order.

Sources and Further Reading

Request a Metal CNC Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Metal CNC chosen.

Request a Quote