A hard anodized coating specified at 0.004 in. (0.10 mm) makes every coated surface grow by half that thickness, so a shaft ground to a diameter of 25.000 mm leaves the bath 0.10 mm larger, and a hole bored to 25.000 mm leaves it 0.10 mm smaller. The specification that says so is MIL-A-8625, and it states the figure in a design note near the end of the document that many buyers never reach.
The standard is the one most often written on a drawing for anodized aluminum, usually as a line of four characters such as “Type II, Class 2”. Those characters stand for a chemistry, a thickness range, a color state and a sealing rule, and each carries consequences for a machined part’s dimensions, its threads and its edges. The sections below read the 1993 revision F, which the US Department of Defense released for public distribution, the way a buyer has to: what the types and classes mean, what a supplier is asked to prove, and what the document leaves to the drawing.
What MIL-A-8625 Covers and What the Types Mean
Revision F covers six types and two classes of electrolytically formed anodic coatings on aluminum and aluminum alloys for non-architectural uses. The types differ by the bath and the weight of the coating: Type I is conventional chromic acid anodizing, Type IB a low-voltage chromic acid process, Type IC a non-chromic acid process offered as a non-chromate alternative, Type II conventional sulfuric acid anodizing, Type IIB a thin sulfuric acid process that is also a non-chromate alternative, and Type III the hard anodic coating.
| Type | Process | Thickness range |
|---|---|---|
| I, IB, IC and IIB | chromic acid, low-voltage chromic acid, non-chromic acid, thin sulfuric acid | 0.00002 to 0.0007 in. (0.5 to 18 µm) |
| II | conventional sulfuric acid | 0.00007 to 0.0010 in. (1.8 to 25 µm) |
| III | hard anodic coating | 0.0005 to 0.0045 in. (13 to 114 µm) |
The thickness ranges are typical ranges and not requirements. For Types I, IB, IC, II and IIB, the requirement is a coating weight, tested before dyeing or sealing, and the thickness a part ends up with is whatever produces that weight on its alloy. For Type III, the requirement is a thickness, and the specification gives a weight to be used in place of it when the buyer prefers.
Types I through IIB are bought by weight and Type III by thickness. A drawing that gives a thickness for a Type II part has asked for something the standard does not control.
What the Chemistries Are For
The specification’s design notes say that Types I, IB and II are intended to improve surface corrosion protection under severe service or to serve as a base for paint systems, and that they can be colored with a large variety of dyes. Types IC and IIB provide non-chromate alternatives where corrosion resistance, paint adhesion and fatigue resistance are required, though they are not suitable replacements where electrolyte entrapment is the main concern. Type III is intended to provide wear and abrasion resistant surfaces with improved corrosion protection, owing to its greater thickness and weight. Applications the document lists for it include valves, sliding parts, hinge mechanisms, cams, gears, swivel joints and pistons.
Coating Weight, Thickness and the Tests Behind Them
For the thin types the requirement is a minimum weight per unit area of unsealed coating, and Table I of the specification sets it.
The weights are these. Types I and IB carry a minimum of 200 mg/ft² (2.2 g/m²). Type IC carries the same minimum with a maximum of 700 mg/ft² (7.5 g/m²). Type II carries a minimum of 1000 mg/ft² (10.8 g/m²). Type IIB carries a minimum of 200 mg/ft² (2.2 g/m²) and a maximum of 1000 mg/ft² (10.8 g/m²).
The maxima on IC and IIB exist for fatigue, according to the design notes, which add that if a higher IIB weight is acceptable for the intended use, Type II should be specified instead. The coating weight is measured by stripping and weighing: the unit weight is the loss on stripping, in milligrams, divided by the area in square feet.
Type III has a default and a tolerance. Unless the contract states otherwise, the nominal thickness is 0.002 in. (51 µm), and it may not vary by more than ±20 % for coatings up to 0.002 in., or by more than ±0.0004 in. (±10 µm) above that. The document adds that thickness of the heavy coating can be controlled to as little as ±0.0001 in. (±2.5 µm) with specialized techniques. For a weight in place of thickness, the specification gives a minimum of 4320 mg/ft² (46.5 g/m²) for every 0.001 in. (25 µm) of unsealed Type III.
The Acceptance Tests
Two tests carry most of the weight. For corrosion resistance, specimens are exposed to a 5 % salt spray test in accordance with ASTM B117, inclined 6 degrees from the vertical, for 336 hours, and are then examined. The requirement is no more than 15 isolated pits in 150 square inches (0.097 m²) of test area from five or more pieces, none larger than 0.031 in. (0.8 mm), and no more than 5 pits in 30 square inches (0.019 m²) from one or more pieces. Type I and IB specimens also may not show patchy dark gray areas, which the design notes read as a sign of coating degradation even when pitting is not visible.
For Type III, unsealed coatings have a wear index limit. The maximum is 3.5 mg per 1000 cycles on alloys with a copper content of 2 percent or higher, and 1.5 mg per 1000 cycles on all other alloys. The design notes add that abrasion resistance decreases as thickness approaches 0.003 in., and that in general it does not rise with thickness.
A thicker Type III coating is not a harder-wearing one. The standard’s own note says wear resistance does not rise with thickness and falls as it nears 0.003 in. (76 µm).
Class 1 and Class 2 for Color
The two classes separate coatings that are not dyed from those that are. Class 1 is non-dyed, and any natural coloration from the anodic treatment on the alloy, or from the sealing process, is not counted as dye. Class 2 is dyed or pigmented by exposure to a suitable solution, with a color and uniformity that the contract or drawing has to specify.
Three limits in the document are worth carrying to a drawing:
- Cast alloys may show dye bleed-out or a lack of color uniformity from their porosity, and the degree of non-uniformity that is acceptable has to be established by the procuring activity.
- Light fastness of dyed coatings is tested only when specified: a delta E of 3 or less after 200 hours of exposure to ultraviolet light, unless the order gives another value.
- Thin types are hard to color, since the design notes say Types I, IB, IC and IIB black anodizing may not be readily obtainable because those coatings are thinner and have a different pore structure.
FED-STD-595 colors may be used as a guide, but the document says they are intended for paint finishes and should be used only for approximate comparison. A color match for a visible part is therefore a conversation about a sample, not a number.
How Anodizing Changes the Size of a Machined Part
The design information section states the growth rule in one sentence: an increase in dimension equal to one half of the thickness of the applied coating can be expected for each surface coated. The document’s own example is a 0.004 in. coating on close tolerance parts, which needs a pre-machining allowance of 0.002 in. (0.05 mm) per surface before hard coating. It recommends placing both a machining dimension and a coated dimension on the drawing.
Threads follow a second rule. All anodic coatings affect thread dimensions, with the major and minor diameters increasing by two times the growth, and the pitch diameter of a 60 degree thread by four times the growth.
| Coating | Growth per surface | External diameter increase | Hole diameter decrease | Pitch diameter increase |
|---|---|---|---|---|
| Type II, 0.0004 in. (10 µm) | 0.0002 in. (5 µm) | 0.0004 in. (10 µm) | 0.0004 in. (10 µm) | 0.0008 in. (20 µm) |
| Type II, 0.0010 in. (25 µm) | 0.0005 in. (13 µm) | 0.0010 in. (25 µm) | 0.0010 in. (25 µm) | 0.0020 in. (51 µm) |
| Type III, 0.002 in. (51 µm) | 0.001 in. (25 µm) | 0.002 in. (51 µm) | 0.002 in. (51 µm) | 0.004 in. (102 µm) |
| Type III, 0.004 in. (102 µm) | 0.002 in. (51 µm) | 0.004 in. (102 µm) | 0.004 in. (102 µm) | 0.008 in. (203 µm) |
A thin Type II coating on a thread already moves the pitch diameter by 20 µm, and a nominal hard coat moves it by 0.10 mm. The specification adds that the coating thickness in small holes and tapped holes can vary from no film to a full normal coating, and that holes over 1/4 in. (6.35 mm) should be anodized. It also states that build-up from anodic coatings, especially Type III, may cause interference on assembly in close fits.
Lapping Hard Coat to Size
Type III coatings generally have increased surface roughness and are less dense on the top surface than in the core, so the document says they may be processed oversized and then lapped or honed to the final dimension. It also notes that hard coatings should generally not be used on parts or portions of parts which normally wear and would need dimensional restoration on rework. Parts with Type II coatings and a total tolerance of 0.0004 in. (10 µm) or less, if lapped, honed or stoned after anodizing, should be treated with QPL-81706 materials to restore surface protection.
Edges, Corners and Fatigue
Because of the way an anodic coating forms, it develops voids at sharp corners and edges. The design notes say sharp edges and corners are difficult to anodize satisfactorily, and that all edges and inside corners should be radiused before anodizing. A chamfer is not recommended unless the resulting sharp edges are radiused as well.
| Nominal coating thickness | Radius of curvature, approximately |
|---|---|
| 0.001 in. (25 µm) | 1/32 in. (0.8 mm) |
| 0.002 in. (51 µm) | 1/16 in. (1.6 mm) |
| 0.003 in. (76 µm) | 3/32 in. (2.4 mm) |
| 0.004 in. (102 µm) | 1/8 in. (3.2 mm) |
A machined pocket whose inside corners are cut by a small cutter has a radius to match the cutter, and the table shows what a hard coat of 0.002 in. (51 µm) wants. The two have to be reconciled in the design, not left to the shop.
The standard is direct about fatigue: the properties of aluminum alloys can be severely reduced by anodic coatings, and as a general rule, the thicker the coating the greater the reduction. It also states that where anodic coatings are required on fatigue critical components, Types I and IB are used because of the thinness of the coating. A part that carries cyclic load and is also hard coated has two requirements that pull against each other.
What the Supplier Signs and What the Drawing Has to Say
The document lets the supplier choose a great deal unless the drawing says otherwise. Process operating conditions are at the supplier’s option. When the coating type is not given, any of Types I, IB, IC, II or IIB may be furnished, and when the class is not given, either Class 1 or Class 2. Parts are anodized after all heat treatment, machining, welding, forming and perforating are complete, and assemblies that would trap electrolyte in joints or recesses are not anodized as assemblies. Heat treatable alloys have to be in the required temper, such as T4, T6 or T73, before anodizing.
The acquisition list in the document asks the buyer to give the following, and a drawing note that skips any of them hands that decision to the supplier:
- The title, number and date of the specification, since later revisions exist and the order has to name the one it means.
- The type and the class, including a Type III thickness where it is not the default 0.002 in.
- Special sealing requirements, since Type III is not sealed where wear resistance is the main function, and is sealed only when the order says so for corrosion.
- Color and uniformity for Class 2, with any light fastness requirement.
- The location of contact marks where it matters to the function of the part.
Alloys the Standard Names
Table V of the specification lists typical minimum thicknesses of Type I, IB, IC and Type II coatings on a set of wrought and cast alloys, among them 6061-T6 and 7075-T6, the two alloys most machined shops cut. The table’s purpose is to show the thickness that would meet the minimum coating weight of Table I on each alloy, so the same weight gives a different thickness on different alloys. The scanned copy opened for this article is too poor to print its figures with confidence, and a buyer who needs them reads them from the standard. The copper and silicon limits in the text are plainer: Type I and Type III are not applied, unless the contract says so, to alloys above 5 percent nominal copper, and Type III is not applied above 8 percent nominal silicon without approval.
What the Standard Leaves Open
The text opened here is a 1993 revision with later amendments and revisions that this article did not open, so a purchase order names the revision. The standard fixes tests and a minimum coating, and it leaves open the exact appearance of two parts from different lots of different alloy. It leaves open, too, how a part that carries a thread fits its mate after coating, which Table 2 answers by arithmetic and the drawing answers by requiring a coated dimension. A buyer who plans a machined part from a first article toward a run of a few hundred can read about low-volume metal CNC and about bridge production before fixing the finish.
Sources and Further Reading
- MIL-A-8625F, Anodic Coatings for Aluminum and Aluminum Alloys, 10 September 1993, US Department of Defense (copy of the ASSIST release for public distribution). https://www.ibiblio.org/apollo/Documents/assist.dla.mil/MIL_A_8625F.pdf
- ASM Material Data Sheet, Aluminum 6061-T6; 6061-T651, ASM International / MatWeb (alloy context). https://asm.matweb.com/search/SpecificMaterial.asp?bassnum=ma6061t6