Flatness of Machined Metal Plates

A plate's measured flatness depends on the stress in its stock, its temperature and its support, as well as on the cut that finished it.

Precision machined aluminum and steel plates with flat fly-cut faces showing a fine circular machining pattern.

A plate of 6061 aluminum 300 mm (11.8 in.) long and 3 mm (0.12 in.) thick, resting on two supports at its ends, sags 54 µm (0.0021 in.) under its own weight. The same plate in 316 stainless sags 55 µm, and in Ti-6Al-4V 54 µm. The three metals differ in density by a factor of three and in stiffness by a factor of three, and the two differences cancel almost exactly, so a flatness reading taken on supports says as much about how the plate lay on the table as about the plate.

Flatness is the tolerance buyers write most casually and shops measure most carefully. On a machined plate it belongs to a face the mill has cut, and it is the cut itself that releases the stock, warms the part and changes how it lies once the clamps come off. A general tolerance supplies a default, and the physics of a thin plate supplies its own opinion. The sections below set the default from ISO 2768-2 beside four effects that move a plate after the last cut: the stress left in the stock, the temperature of the plate and its surroundings, the way it is supported, and the shop’s choice of when to relieve it.

What Flatness General Tolerances Allow

A machined plate leaves the mill with faces cut flat. Where the drawing gives a face no flatness of its own, ISO 2768-2 sets the tolerance it is held to. The standard sets general tolerances on straightness and flatness in three classes, H, K and L, for ranges of nominal length. The standard’s 1989 public sample prints the flatness table, and the figures below are read from it. The table gives one value for each length range, with no plus and minus around it.

Table 1. ISO 2768-2 general tolerances on straightness and flatness, in mm with inch in brackets, from Table 1 of the standard’s 1989 public sample
Nominal length H K L
up to 10 mm (0.39 in.) 0.02 (0.0008 in.) 0.05 (0.0020 in.) 0.1 (0.0039 in.)
over 10 up to 30 mm (1.18 in.) 0.05 (0.0020 in.) 0.1 (0.0039 in.) 0.2 (0.0079 in.)
over 30 up to 100 mm (3.94 in.) 0.1 (0.0039 in.) 0.2 (0.0079 in.) 0.4 (0.0157 in.)
over 100 up to 300 mm (11.8 in.) 0.2 (0.0079 in.) 0.4 (0.0157 in.) 0.8 (0.0315 in.)
over 300 up to 1000 mm (39.4 in.) 0.3 (0.0118 in.) 0.6 (0.0236 in.) 1.2 (0.0472 in.)
over 1000 up to 3000 mm (118 in.) 0.4 (0.0157 in.) 0.8 (0.0315 in.) 1.6 (0.0630 in.)

Two features of the table are worth carrying around. Each class doubles the one before it, so K is twice H and L twice K at every length. And the allowance grows by steps that are much smaller than the length: from 100 mm to 300 mm in class H the length triples while the allowance doubles, from 0.1 to 0.2 mm.

A general flatness class applies to every face without its own flatness callout. A plate that has to seal, slide or mount a sensor carries a flatness tolerance of its own on the drawing.

What the Default Does Not Cover

A drawing that quotes ISO 2768-K for a plate of 250 mm length accepts 0.4 mm (0.016 in.) of flatness error. That is 400 µm, which is more than seven times the self-weight sag worked out below for a thin plate, and many times the amount that a sealing face or a rail seat allows. The summaries opened for this article do not state which instrument checks flatness or on what supports, and the drawing is where those are named.

Stock Stress and the Temper of the Plate

A plate is rolled, solution treated, quenched and then aged. The quench cools the surface first, and the core shrinks later against a surface that has already set, which locks in stress. When a pocket is cut, material that was holding the stress is removed, and the plate moves to a new balance. A clamped plate cannot show that movement until it is released, so the face that carries the flatness callout is the one to finish last, with light passes after the heavy cuts, when the plate has already found its new shape.

The temper designation tells the buyer what the mill did about it. An aluminum temper chart defines T651 as solution heat treated, stress relieved by stretching and artificially aged, equivalent to T6 and applying to plate and rolled bar, and defines T6511 as the same with minor straightening for extruded rod, bar and shapes. A paper abstracted by ASM on 7075 states that the stress left by the quench is relieved by a later stretching step, and that its distribution through the thickness was measured by removing layers. The same abstract reports a difference between the distortion measured and the stress calculated, so a stretched plate is not guaranteed flat after machining, only more likely to be.

The ASM data sheets for 6061 and 7075 both carry the pair of designations T6 and T651 on the same set of typical properties, which is why the property tables cannot tell a buyer which one the plate is. The purchase order has to name it.

Stress Relief on Titanium and Heat-Treated Stock

For titanium, ATI prints a stress relief anneal of 538 to 649 °C (1,000 to 1,200 °F) for 1 to 8 hours, and Zapp gives a stress relief of about 500 to 650 °C. Both place it as a treatment of the part, and a common sequence for a thin or flat part is to rough it, relieve it and then finish it, so that the stress released by roughing does not move the finished face. The sheets do not prescribe that order, and it is a decision for the drawing or the shop’s process plan.

Face Milling, Flipping and the Finishing Pass

The machining sequence is where a shop turns these effects into a flat face. A plate is usually face milled or fly-cut on one side, turned over and cut on the other, so that the stress released by each heavy cut is balanced by a cut on the opposite face. The roughing passes take the bulk of the stock from both sides, the clamps are then loosened so the plate can settle, and the face that carries the flatness callout is finished last with light passes.

Fixturing decides how much of that settling the face shows. Heavy clamps hold a bowed plate flat while it is cut, and the face springs back when they come off, so the finishing pass is taken with the plate held lightly, on supports that do not force it. Where the drawing asks for a stress relief, it goes between the roughing and the finishing passes, as the titanium sequence above describes, and not after the last cut on the critical face, since that cut is the one the relief is meant to protect.

Heat and the Bow of a Machined Plate

Heat is the second cause, and on the mill it comes from the cut. Face milling and fly-cutting put heat into the top face while the clamped underside stays near the temperature of the table. A face that sits warmer than the face opposite it grows longer, and a thin plate bends to accommodate it. For a simple strip with a linear temperature difference across its thickness, the curvature is the expansion coefficient times the difference, divided by the thickness, and the sag over a span is the curvature times the span squared over eight.

Take a through-thickness difference of 2 °C, a 300 mm span and the expansion coefficients from the datasheets opened for these resources: 23.6 µm/m·°C for 6061-T6, 16.6 for 316 and 8.6 for Ti-6Al-4V.

Table 2. Bow of a 300 mm (11.8 in.) plate from a 2 °C temperature difference between its faces, in µm with inch in brackets, from the simple strip model
Material 3 mm (0.12 in.) thick 5 mm (0.20 in.) thick 10 mm (0.39 in.) thick
6061-T6 aluminum 177 (0.0070 in.) 106 (0.0042 in.) 53 (0.0021 in.)
316 stainless 124 (0.0049 in.) 75 (0.0030 in.) 37 (0.0015 in.)
Ti-6Al-4V 64 (0.0025 in.) 39 (0.0015 in.) 19 (0.0007 in.)

The 3 mm aluminum plate bows 177 µm, nearly the whole class H flatness allowance of 0.2 mm for its length. Thickness divides the bow directly, so a plate twice as thick bows half as much, and a material with a lower coefficient of expansion bows less. A 2 °C difference is a small one, and a plate on a cold machine table under a cutter can plausibly see more. That is one reason the finishing pass comes after the plate has settled to the temperature of the shop.

The model is a textbook one and it leaves out clamping, edge effects and the way heat enters the plate, so the numbers are indications. They are enough to show which way each variable moves.

Support on the Table and on the Inspection Plate

The third effect is gravity and support, first on the machine table and then on the inspection plate. Clamped flat on the table or a vacuum fixture, a thin plate is cut while it is held straight. The way it is supported once released decides what is measured. A plate resting on two end supports sags under its own weight, and the sag depends on the density, the modulus, the span and the thickness. For a plate of unit width the midspan deflection is 5 × density × g × thickness × span⁴ divided by 384 × modulus × the second moment of area, which for a rectangular section is thickness cubed over 12.

Table 3. Self-weight sag of a 300 mm (11.8 in.) plate on two end supports, in µm with inch in brackets, from densities and moduli on the ASM, Cleveland-Cliffs and ATI sheets
Material Density and modulus 3 mm thick 5 mm thick 10 mm thick
6061-T6 aluminum 2.70 g/cm³, 68.9 GPa 54 (0.0021 in.) 19.5 (0.0008 in.) 4.9 (0.0002 in.)
316 stainless 8.03 g/cm³, 193 GPa 57 (0.0022 in.) 20.7 (0.0008 in.) 5.2 (0.0002 in.)
Ti-6Al-4V 4.47 g/cm³, 113.8 GPa 54 (0.0021 in.) 19.5 (0.0008 in.) 4.9 (0.0002 in.)

The three rows are nearly identical because the ratio of density to modulus is nearly the same for the three metals, between 0.039 and 0.042 g/cm³ per GPa. Thickness matters far more than the metal. Going from 3 mm to 5 mm cuts the sag to a little over a third, and going to 10 mm cuts it to about a ninth.

The self-weight sag of a plate depends on its thickness and span, and hardly on which of these three metals it is made from. A thin plate checked on end supports reads about 54 µm lower in the middle than the same plate checked on a flat surface.

Which Way the Plate Is Measured

The result for an inspector is practical. A plate measured lying flat on a surface plate and the same plate measured on edge supports read differently by the amount in Table 3. A thin plate whose drawing tolerance is 0.05 mm (0.002 in.) can fail the check on supports and pass it on a plate, with no change in the part. The drawing or the inspection plan names the support, and a report that states it can be repeated.

Coatings After the Cut

MIL-A-8625F directs that parts are anodized after machining, forming and heat treatment are complete, so a coating follows the flatness measurement and not the other way round. A uniform coating grows each face by half its thickness and moves no plane relative to the other. A coating that varies does: the same document allows a Type III coating of 0.002 in. (51 µm) to vary by ±20 %, which is ±10 µm on a face. For a plate held to 0.05 mm (0.002 in.), thickness variation of that size is a fifth of the tolerance, and it is a reason to state on the drawing whether the flatness applies before or after coating.

Span and Thickness Set Both Effects

The two physical effects scale differently with the plate’s proportions, and the proportions decide how the plate is clamped and supported on the mill. The bow from a temperature difference grows with the square of the span and falls with the thickness, while the self-weight sag grows with the fourth power of the span and falls with the square of the thickness. Doubling the span of the 3 mm aluminum plate from 300 mm to 600 mm (23.6 in.) takes the bow from 177 µm to 708 µm, and the sag from 54 µm to about 865 µm.

The sag then exceeds the class H allowance for its length range, which is 0.3 mm (0.012 in.) for lengths over 300 up to 1000 mm. A long thin plate is therefore a different problem from a short one, and the general class does not say so. A part that is only a flat outline in thin stock, with no pocket and no machined face, is usually not a milling job at all. It is cut from sheet by laser cutting and keeps the flatness of the sheet as rolled, and it comes to the mill when a face, a pocket or a tight flatness note needs the cut. For such plates the drawing states the thickness, the support and the temperature along with the flatness, and the supplier reports them with the result.

One Plate Through the Four Effects

Take a plate of 6061-T651, 200 mm by 200 mm and 6 mm (0.24 in.) thick, with a drawing that says ISO 2768-H. The length of 200 mm falls in the over 100 up to 300 mm row of Table 1, so the general allowance is 0.2 mm (200 µm). The same strip models give two numbers for it. Resting on two end supports it sags 2.7 µm under its own weight, and with a 2 °C difference between its faces it bows 39 µm.

Those two effects together take about a fifth of the class H allowance, which leaves room for the stress that remains in the stock. If the plate is a T6 plate and not a T651, nothing in the opened sources says how much of the allowance the stress takes, and that is the number a trial cut answers. If the drawing asked for 0.05 mm (0.002 in.) of flatness instead of 0.2 mm, the thermal bow alone would take 78 % of it, and the plate would have to be measured at a controlled temperature on a defined support.

The same arithmetic runs the other way for a stiff, thick part. A 10 mm plate of the same length and temperature difference bows 23.6 × 10⁻⁶ × 2 ÷ 10 × 200² ÷ 8 = 24 µm, and sags 1.0 µm under its weight, so for a thick plate the general tolerance is comfortable and the question moves to the stock and the cutting sequence. That sequence is the one laid out above: rough both faces, release the clamps so the stock stress shows, flip the plate and take skim cuts on each side before the finishing pass.

Setting a Flatness Tolerance That Can Be Checked

Combining the four effects gives a simple procedure for a drawing, and a short list of what to state with it.

  • The tolerance itself, in a callout of its own for any face that matters, with the general class left to the rest.
  • The stock temper, T651 or the equivalent stress-relieved temper, for plate that is cut deeply.
  • The sequence, for titanium and heat-treated stock, naming the stress relief between roughing and finishing.
  • The thickness, since a thin plate can use up a tolerance by bowing or sagging without any fault in the machining.
  • The inspection condition, the support and the temperature, so the number is repeatable.

For the 3 mm aluminum plate against the class H allowance of 0.2 mm (200 µm) for its length range, the shares are plain. Self-weight sag on end supports of 54 µm takes 27 %, the bow from a 2 °C difference between faces of 177 µm takes 89 %, and the two together, if they add, come to 231 µm or 116 % of the allowance.

A plate that passes comfortably in the machine can fail in the inspection room for reasons that have nothing to do with the cut. For quantities from a first part to a short run, the sensible plan is to fix the support, the temperature and the temper once, and to carry them through every lot. A buyer sequencing that run can read about low-volume metal CNC and about bridge production before fixing the flatness note.

Sources and Further Reading

Request a Metal CNC Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Metal CNC chosen.

Request a Quote