How Many Parts One Cutting Edge Makes in a Machined Run

The parts an edge makes equal its minutes of life divided by the minutes each part spends on it, so a faster cycle can use more edges than it saves.

Square uncoated grey carbide indexable cutting inserts, plain grey carbide with no coating colour, new ones with sharp edges and worn ones with dull flank wear, beside small machined steel parts.

A turning insert is retired when its flank wear reaches about 0.3 mm, a figure used as the wear criterion in a Lund University and Seco Tools study of eleven material and tool combinations. That is the width of three sheets of printer paper worn into the face of a carbide edge, and it is the quantity that sets how many parts one corner of an insert can cut. Everything else in the count follows from it: the speed that reaches the limit in a given number of minutes, the minutes each part spends in contact with the tool, and the number of edges a lot uses up.

For a buyer, the edge count looks like a detail of the shop floor. It is also the reason a lot of 50 can run on one setup of tools and a lot of 1,000 needs a plan for changing them, and the reason a faster cycle does not always give more parts per day. This piece follows the arithmetic from the wear limit to the edges a lot consumes, with the published models and an assumed worked case.

What Decides How Many Parts a Cutting Edge Can Make

Parts per edge is a quotient. The numerator is the tool life, the minutes a cutting edge can stay in contact with the workpiece before it reaches the wear criterion. Cutting time per part on that edge is the denominator. Tool life depends on the cutting speed above all, then on the chip thickness, which comes from feed and depth of cut, and on the tool and workpiece material.

The Lund study states the dependency in its introduction: a tool life model takes cutting speed, depth of cut, feed and tool geometry as inputs, along with the machinability of the work material and the tool material and design, and returns an estimated time in cut for a chosen wear criterion. In the study, the named criteria are a maximum flank wear of 0.3 mm or a maximum crater wear of 0.5 in the paper’s units.

Parts per edge equals the minutes an edge lasts divided by the minutes each part spends on it. Speed shortens the first number and the second number together, and they do not shrink at the same rate.

The best-known relation, from F. W. Taylor in 1906, ties cutting speed to tool life: the speed multiplied by the tool life raised to a constant exponent equals a constant. The paper notes that speed is the most influential factor, feed matters less, and depth of cut plays a minor role because the load is spread over a longer length of edge.

Rarely does a part meet a single tool. A turned shaft meets a roughing insert, a finishing insert, a grooving tool and a drill, each with its own life, so the lot’s edge count is a list with one line per tool and the tool that runs out first sets the rhythm of interruptions. Roughing tools reach the wear limit on the heavy cuts, finishing tools on the cuts where a small wear width already changes the size and the surface of the part.

One Edge Is One Corner of an Insert

An indexable insert has several cutting corners, and each is an edge in this count. A square insert with four corners gives four edges per insert, so the tool changes of a lot are counted in edges while the shop’s purchase records count inserts. For a solid carbide end mill, the tool life is a single number that ends at the regrind or the bin.

Wear Types That End an Edge Early

A tool life number assumes the edge wears the way the model expects, along the flank, and it is retired at the stated wear width. Other wear types end an edge earlier and less predictably. Sandvik Coromant’s page on wear on cutting edges lists seven and names the cause of each.

Table 1. Wear types on cutting edges and their causes, as listed by Sandvik Coromant
Wear type Cause given by the maker Where it shows
Flank wear Abrasion from hard constituents in the workpiece Preferred wear type, with predictable and stable tool life
Crater wear Chemical reaction between workpiece and tool, increased by cutting speed Rake side of the insert
Built-up edge Chip material pressure-welded to the edge Most common with sticky materials such as low carbon steel, stainless steel and aluminum
Notch wear Adhesion and a deformation-hardened surface Rake face and flank at the depth-of-cut line, common in stainless steels and heat-resistant alloys
Plastic deformation Edge softened by cutting temperature above what the grade withstands Not described on the page
Thermal cracks Swings from hot to cold, fast, typical of interrupted cuts Cracks across the edge, worse with coolant on milling
Edge chipping and breakage Mechanical overload, including chip hammering, excess depth of cut or feed, built-up edge and vibration Not described on the page

Tool life models describe the first row. The other six explain why a shop’s real edge count can fall short of the calculated one. Built-up edge appears at low cutting speed on aluminum and stainless steel, which is the opposite of what a simple “slower is gentler” rule suggests. Notch wear sits at the depth-of-cut line, so a part with a surface hardened by the previous pass wears the edge at one point, and a longer life at the average does not help.

Wear shows up in the part before it shows in the tool. A worn edge raises cutting force, and in aluminum machining studies a worn tool gives larger entrance burrs and bigger burrs overall. Edge condition is therefore a quality input as well as a count.

Models of Tool Life and How Far They Can Be Trusted

The Lund study tested the common tool life models on turning data: 235JRG2, 16MnCr5, C45E, 42CrMo4, 100Cr6 and X5CrNi18-9 stainless in groups P and M, and EN-GJS-500-7 cast iron in group K. Five or more tests were run per material and tool grade, varying cutting data across a window suited to the insert’s geometry and chip breaker. The wear of each tool was measured under an optical microscope.

Table 2. Average model error against the measured turning data, Johansson and colleagues, Procedia Manufacturing 11
Model Inputs Average error
Colding (plain) Equivalent chip thickness, 5 constants About 4.0 %
Extended Taylor Equivalent chip thickness, 3 constants 10.8 %
Extended Taylor Feed and depth of cut, 4 constants 11.9 %
Taylor Cutting speed only, 2 constants 17.9 %
Taylor, mid-range data only Cutting speed only 11.3 %
Extended Taylor, mid-range data only Feed and depth of cut, or equivalent chip thickness 3.9 %

Two lessons come out of the table. A model with more inputs fits better across a wide range of cutting conditions. And the simple model works acceptably inside a narrow window: with the extreme data points removed and the span of chip thickness reduced, the error of the Taylor model fell from 17.9 % to 11.3 % and the extended versions to 3.9 %.

The authors conclude that the Taylor models are relatively accurate when used with caution and in smaller ranges of chip thickness. For a shop adjusting cutting data in an existing process, with tool selection fixed, the standard Taylor model may well be good enough, and it needs only two to four test points.

Where the Models Stop Being Reliable

Models performed less well on the high alloy steels and the stainless steel in the study. The authors note that these materials work-harden the surface left by the previous cut, which matters more when the chip is thin, as it is in finishing. A model fitted on roughing data and extrapolated to finishing in stainless steel is a poor basis for an edge count.

The study also states that a normal range of equivalent chip thickness can be about 10 times the smallest value when covering roughing through fine finishing. A tool life figure belongs to a combination of material, grade, speed, feed and depth of cut, and it does not transfer to another combination.

Material Groups and the Count

The Lund paper says metal machining divides work materials into six ISO groups: P for steel, M for stainless steel, K for cast iron, N for aluminum, S for heat-resistant alloys and H for hardened steel. The study covered only P, M and K. Its numbers therefore do not carry over to aluminum or to titanium and nickel alloys, and a count taken from turning steel should not be applied to a part in another group.

The paper also points to a practical limit on the way catalogues are drawn. Published cutting data is often extended as a straight line to the left of a certain chip thickness, so the speed does not fall as the chip gets thinner. The authors found no scientific proof that tool wear in finishing behaves that way, and they advise great care before publishing fine finishing data on that basis. For a buyer, the point is that a finishing pass on a tight surface specification is the cut least likely to behave as the catalogue says.

A Worked Case With Assumed Numbers

An assumed case shows how the count behaves. Assume a shop turning a part from a steel bar. A first test shows an edge lasting 40 minutes at a cutting speed of 200 m/min (656 ft/min), and a second shows 20 minutes at 260 m/min (853 ft/min). These values are chosen for arithmetic and are not data for a real part.

Fitting the Taylor relation to the two points gives an exponent of 0.38, from the ratio of the logarithms of the speeds and of the lives. The relation then predicts about 15 minutes of life at 290 m/min. Each part needs 4.0 minutes of contact at 200 m/min, which scales to 3.08 minutes at 260 m/min because the same length of cut takes less time at a higher speed.

Table 3. Edges used for lots of different sizes at the two assumed speeds
Lot size Edges at 200 m/min (10 parts per edge) Edges at 260 m/min (6.5 parts per edge)
10 parts 1 2
50 parts 5 8
200 parts 20 31
1,000 parts 100 154

Raising the speed by 30 % shortens each part’s cutting time by 23 % and cuts the parts per edge from 10 to 6.5. Over a lot of 1,000, the lower speed uses 100 edges and the higher one 154. Time gained on each part is lost again at every tool change, and whether the lot finishes sooner depends on how long a change takes against how much cutting time the faster speed saves.

A faster cycle consumes edges faster than it saves minutes. The number to compare is the time per part including the share of every tool change, not the cutting time alone.

Lot Size and the Cost of a Tool Change in Minutes

A tool change takes machine time, and the same assumed numbers show where it tips the balance. Take the lot of 1,000 parts. At 200 m/min each part spends 4.0 minutes in cut, so the lot cuts for 4,000 minutes and uses 100 edges. The higher speed of 260 m/min brings each part to 3.08 minutes in cut, so the lot cuts for 3,077 minutes and uses 154 edges.

Add a change time to each edge, and the totals diverge. Suppose a change, with its offset update and first-part check, takes 3 minutes: the slower lot then runs 4,300 minutes and the faster 3,539. At 17 minutes per change the two totals meet, and at longer changes the slower speed finishes first. The break-even is the extra cutting time saved, 923 minutes, divided by the 54 extra changes. Every figure rests on the assumed 40 and 20 minute tool lives, so they show the method and carry no meaning for a real part.

Three readings follow from the arithmetic.

  1. A faster setting pays when a tool change is quick, as with indexable inserts changed at the machine, and stops paying when a change is slow, as when a tool has to be re-measured or a fixture re-seated.
  2. Short lots hardly feel the difference. A lot of 10 parts uses 1 or 2 edges, and the change time is a small share of the run.
  3. Long lots feel it strongly, and the edge count is the first place to look when the cycle time per part on a long run is higher than the cutting time alone would give.

A shop that tracks edges per lot can tell a buyer which speed it settled on and why. The reason is more useful than the number, since the right speed moves with the cost of a change on that machine.

Tool Changes Inside a Run and How an Order Can Handle Them

Mid-lot, a tool change interrupts the process. A new edge is not the old edge: its position in the holder can differ by a small amount, so the offset is updated, and the first part after the change is measured before the lot continues.

  • A life count by parts. A shop can retire an edge after a set number of parts, set below the calculated life, so that a hardened surface does not push the edge past its wear limit. An order can ask for the count used.
  • Offsets after each change. The edge’s size shift goes into the tool offset, either by touch probe in the machine or by a measured part.
  • Check of the first part after a change. A part measured at the critical features after each change shows a bad edge seating before many parts follow.
  • Records of the edge count. The number of edges used for a lot is a plain record of whether the cycle was stable or struggling.

Where a part has a surface finish or a tolerance that a worn edge would break, the retire point is set by the part, not by the tool, and the edge count rises accordingly.

A lot that is short enough to run on one edge per operation behaves differently from one that uses a hundred. In a lot of the first kind, the question is whether the edge is sharp and the setup checked. In the second, the question is the planned count, the change procedure and the evidence from the first parts of each edge. Moving from the first kind to the second is the point at which a run from low-volume CNC machining turns into bridge production, and the edge count is part of what carries over.

Sources and Further Reading

Request a Metal CNC Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Metal CNC chosen.

Request a Quote