ExpansionData SheetHardness

6061-T6 and 7075-T6 Aluminum for CNC Machined Parts

Both alloys machine into the same shapes, but strength, temper and thermal growth decide which one holds a drawing's dimensions and loads.

CNC machined aluminum parts in two alloys, pocketed rectangular blocks and ribbed brackets, the 6061 ones satin silver and bead-blasted, the 7075 ones a slightly brighter machined silver with fine tool marks.

On the same 0 to 100 scale of aluminum alloys, ASM scores the machinability of 6061-T6 at 50 and of 7075-T6 at 70. The same two data sheets put tensile strength at 310 MPa (45,000 psi) for the first and 572 MPa (83,000 psi) for the second. A buyer who reads only those four figures could conclude that the stronger alloy is also the easier one to cut, and the sheets do nothing to prevent that reading.

The numbers are accurate, yet each of them answers a narrower question than it appears to. Strength is a property of the temper, machinability is a rating without a stated method, and the stiffness that decides how a thin wall behaves is almost identical in both alloys. What follows reads the two ASM sheets side by side, adds the temper designations that appear on a purchase order, and turns the thermal figures into millimeters on a part.

6061-T6 and 7075-T6 Compared on the Datasheet

The two alloys sit in different families. 6061 is a magnesium and silicon alloy of the 6000 series, with 0.8 to 1.2 % magnesium and 0.4 to 0.8 % silicon. 7075 belongs to the 7000 series, with 5.1 to 6.1 % zinc, 2.1 to 2.9 % magnesium and 1.2 to 2.0 % copper. Those percentages are the Aluminum Association composition limits printed on the ASM sheets, and the second alloy’s copper and zinc are what buy its strength.

Table 1. Typical properties of 6061-T6 and 7075-T6 in dual units, as printed on the ASM Material Data Sheets (Aluminum Association typical values, listed there as not for design)
Property 6061-T6 7075-T6
Density 2.70 g/cm³ (0.0975 lb/in³) 2.81 g/cm³ (0.102 lb/in³)
Ultimate tensile strength 310 MPa (45,000 psi) 572 MPa (83,000 psi)
Tensile yield strength 276 MPa (40,000 psi) 503 MPa (73,000 psi)
Elongation at break, 1.6 mm (1/16 in.) sheet 12 % 11 %
Elongation at break, 12.7 mm (1/2 in.) diameter 17 % 11 %
Brinell hardness, 500 g load, 10 mm ball 95 150
Shear strength 207 MPa (30,000 psi) 331 MPa (48,000 psi)
Fatigue strength, 500,000,000 cycles, completely reversed 96.5 MPa (14,000 psi) 159 MPa (23,000 psi)
Modulus of elasticity 68.9 GPa (10,000 ksi) 71.7 GPa (10,400 ksi)
Thermal conductivity at 25 °C (77 °F) 167 W/m·K 130 W/m·K
Linear expansion, 20 to 100 °C (68 to 212 °F) 23.6 µm/m·°C 23.6 µm/m·°C
Melting range 582 to 652 °C (1080 to 1205 °F) 477 to 635 °C (890 to 1175 °F)
Machinability, 0 to 100 scale of aluminum alloys 50 % 70 %

Read as ratios, the table says something compact. The 7075 figures run about 1.8 times higher for tensile and yield strength, 1.6 times higher for hardness and fatigue strength, and 1.5 times higher for shear. Density is only 4 % higher, so the strength-to-weight advantage is real, at roughly 204 MPa per g/cm³ against 115 for 6061 when ultimate strength is divided by density.

Strength roughly doubles between the two alloys, while stiffness moves by 4 % (68.9 against 71.7 GPa). A part that is too flexible in 6061 stays too flexible in 7075, and only a change of geometry fixes that.

Stiffness in Practice

The 4 % difference in modulus has a concrete meaning for a rib or a wall. The deflection of a beam under a given load falls with the cube of its depth, so a 6061 rib that needs to be half as flexible has to be deeper by the cube root of two, about 26 %. Switching the same rib to 7075 buys 4 % less deflection, which is the equivalent of 1.3 % more depth. A designer who changes alloy to cure a flexing wall is spending strength on a problem that depth solves directly.

Bearing, Notch and Heat Treatment Figures

The 6061 sheet carries three rows that the 7075 sheet lacks, and they are the ones a pinned or bolted joint reads. Ultimate bearing strength is 607 MPa (88,000 psi) and bearing yield strength 386 MPa (56,000 psi), both at an edge distance to pin diameter ratio of 2.0. Notched tensile strength is 324 MPa (47,000 psi) on a side-notched specimen 2.5 cm wide and 1.6 mm thick with a stress concentration factor of 17. A designer who wants the equivalent for 7075 has to find it in another source, and the absence of a row is not evidence of a lower figure.

The processing rows explain the tempers in temperature terms. 6061 is solution treated near 529 °C and aged at 160 °C for 18 hours in rolled or drawn product, or at 177 °C for 8 hours in extrusions and forgings. 7075 is solution treated at 466 to 482 °C and aged at 121 °C. The T6 designation is the result of those two steps and is not something a machine shop adds or removes.

What the Sheets Do Not Say About Elongation

The two elongation rows are the only place where the sheets disagree with a simple ranking. 6061-T6 stretches 12 % in 1.6 mm sheet and 17 % in 12.7 mm round bar, while 7075-T6 stays at 11 % in both. The stronger alloy is therefore the less forgiving one in a local overload, and a machined part with a sharp internal corner or a cross hole has nowhere to spread that stress.

Fracture toughness points the same way. ASM prints 29 MPa·m½ (26.4 ksi·in½) for 6061-T6 in the TL orientation, while 7075-T6 is listed at 20, 25 and 29 MPa·m½ in the S-L, T-L and L-T directions. The best direction of 7075 equals the single figure for 6061, and its weakest direction is a third lower. Orientation is something a drawing can control, since the grain of a plate or bar runs one way and the part is cut out of it in whatever direction the nesting allows.

What T6, T651 and T6511 Mean on a Purchase Order

The data sheet title for each alloy carries two designations, 6061-T6 and 6061-T651, 7075-T6 and 7075-T651, and the properties printed under them are one set. That is deliberate. An aluminum temper chart defines T651 as solution heat treated, stress relieved by stretching and artificially aged, equivalent to T6 in properties, and applying to plate and rolled bar. T6511 carries the same treatment with minor straightening and applies to extruded rod, bar and shapes.

Table 2. Temper designations that appear for these two alloys, as defined in an aluminum temper designation chart
Designation Treatment Product form
T6 solution heat treated, artificially aged any wrought product
T651 solution heat treated, stress relieved by stretching, artificially aged; equivalent to T6 plate and rolled bar
T6511 as T651, with minor straightening after stretching extruded rod, bar and shapes
T7351 solution heat treated and specially artificially aged for stress corrosion resistance 7075 sheet and plate

The extra digit matters at the machine and not on the tensile test. A plate that was quenched from solution temperature carries stresses locked in by the uneven cooling, and a pocket cut out of it releases them unevenly. A paper abstracted by ASM on 7075 states that the residual stress produced by quenching is relieved by a later stretching step, and that the authors measured its distribution through the thickness by removing layers. The same abstract points out a difference between the distortion measured and the stress calculated, so stress relief reduces the risk without removing it.

For a drawing, the practical consequence is to name the temper in full. “7075-T6” on a plate-cut part leaves the supplier free to quote from any T6 stock, while “7075-T651” asks for the stretched product. A buyer who sees a bowed flat part come back from a one-sided pocket has a first question to ask, and it is which temper the plate was.

The Overaged Temper for Stress Corrosion

T7351 appears in the chart because it changes the property set. Alcoa’s note on the ASM 7075 sheet states that the T7351 temper offers improved stress-corrosion cracking resistance. The trade for that treatment is a lower strength than T6, which the sheets for T6 do not print, so a drawing that needs both the T7351 behavior and the T6 strength figures has to be checked against a sheet for T7351 itself. That last row is also where a long part can change process: a part of constant section can be ordered as an aluminum extrusion in 6061-T6511, with only its ends, holes and pockets machined, instead of the whole section being cut from plate.

Machinability Ratings and What the Number Leaves Out

The 50 and 70 in Table 1 are positions on a scale of aluminum alloys, and the sheets name no test method, no tool and no cutting speed. A rating of this kind compares alloys with one another, and says nothing about whether a particular part will cut cleanly. The ASM sheet for 6061 adds a second kind of statement: that the T8 and T9 tempers offer better chipping characteristics than T6. Chip form is a machining property that a single index cannot express.

Several things sit outside a rating and inside the work order:

  • Chip formation, which sets how much heat leaves with the chip and whether long strings wrap the tool; the sheets state a preference for tempers T8 and T9 over T6 on this count for 6061.
  • Residual stress, which moves a thin part after the last cut and which the T651 designation reduces.
  • Hardness, 95 against 150 Brinell on the sheets, which sets how fast an edge dulls on a long cut.
  • Melting range, 582 °C at the lowest for 6061 and 477 °C for 7075, a reminder that a dull tool or a starved coolant supply heats a metal whose solidus sits below 600 °C.

A machinist chooses cutting data from the tool maker, not from a data sheet for the alloy. The alloy sheet fixes the boundaries, and the cutter supplier fills in the speeds.

The 0 to 100 machinability index ranks alloys against each other on an unstated test. It cannot tell a buyer which one holds flatness after a pocket or which one leaves a clean thread.

Heat, Expansion and Measuring at 20 °C

Both alloys expand 23.6 µm per meter per °C over 20 to 100 °C on the ASM sheets, so expansion never separates them. It still shapes the measurement. A part 200 mm (7.87 in) long that warms by 20 °C grows 23.6 × 10⁻⁶ × 200 × 20 = 0.094 mm (0.0037 in), nearly the whole width of a ±0.05 mm tolerance band.

Table 3. Growth of an aluminum part with temperature, from the 23.6 µm/m·°C coefficient of the ASM sheets, 6061-T6 and 7075-T6 alike
Length 5 °C warmer 10 °C warmer 20 °C warmer
50 mm (1.97 in) 0.006 mm (0.0002 in) 0.012 mm (0.0005 in) 0.024 mm (0.0009 in)
100 mm (3.94 in) 0.012 mm (0.0005 in) 0.024 mm (0.0009 in) 0.047 mm (0.0019 in)
200 mm (7.87 in) 0.024 mm (0.0009 in) 0.047 mm (0.0019 in) 0.094 mm (0.0037 in)
400 mm (15.7 in) 0.047 mm (0.0019 in) 0.094 mm (0.0037 in) 0.189 mm (0.0074 in)

A part cut warm and measured cold shrinks to its true size on the table, which is why a shop that holds tight dimensions on aluminum lets the part and the gauge rest at room temperature before the check. The point matters for any metal, and aluminum has less margin than most: Carpenter prints 10.4 × 10⁻⁶ per °F, about 18.7 µm/m·°C, as the mean expansion of 303 stainless, so aluminum at 23.6 grows about 26 % more per degree. Thermal conductivity cuts both ways: 6061 at 167 W/m·K sheds heat 28 % faster than 7075 at 130 W/m·K, so a finishing cut on 7075 holds its heat a little longer in a thin section.

Four Questions Before Quoting a Dimension

Four questions cover most of it. At what temperature will the part be measured, and was the drawing tolerance stated for 20 °C? Does the feature span a long dimension, where 0.047 mm per 100 mm per 20 °C begins to eat the tolerance? Is the mating part another alloy, such as 303 stainless at about 18.7 µm/m·°C, so the fit changes between the shop and the field? And will the part see temperatures above room temperature in service, where its growth is a design input and not a measurement artifact?

Choosing Between the Two for a Given Part

Reduced to a decision, the two alloys separate on what the part has to carry, and the sheets support five usable tests.

  1. Load and fatigue, where 7075’s 159 MPa fatigue strength at 500 million cycles against 96.5 MPa for 6061 decides most structural cases.
  2. Stiffness, where the 4 % difference in modulus means geometry has to carry the load.
  3. Coating and finishing, where the 6061 sheet’s own note of good acceptance of applied coatings is the one finishing statement either sheet makes, and the finish standard named on the drawing has to be checked with the supplier against the alloy.
  4. Joining, where the 6061 sheet lists excellent joining characteristics and the 7075 sheet makes no such statement.
  5. Stress corrosion in service, where the T7351 temper of 7075 exists to address it.

Heavier-duty uses that the sheets list for 7075 include aircraft fittings, gears and shafts, worm gears and defense parts. For 6061 the sheet lists camera lens mounts, couplings, marine fittings, valve parts and hinge pins. The lists overlap on aircraft fittings, which is a reminder that the choice is made per part and not per industry.

What a Supplier Signs and What Stays Open

A mill certificate for plate states the alloy, the temper and the lot, and the typical values of Table 1 are not what it guarantees. The Aluminum Association figures on the ASM sheets are labeled typical and not for design, so a design calculation takes its minimum values from the specification the material is bought to, and the drawing names that specification. Directional properties, residual stress and the real elongation of a thick section stay open until a test on that lot closes them.

A property table is a description of the alloy. A purchase order, with alloy, temper, product form and specification all named, is what turns it into a part.

For quantities from a single first part to a few thousand, the choice of 6061 or 7075 is made once and carried through the whole run, and a change of alloy partway through a bridge run changes stiffness, finish response and dimensions together. A buyer planning that sequence can read about low-volume metal CNC and about bridge production before settling the alloy.

Sources and Further Reading

Request a Metal CNC Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Metal CNC chosen.

Request a Quote