DrawingGaugeCertificate

Machining C36000 Free-Cutting Brass for Turned Parts

C36000 cuts so freely that spindle speed, chip control and finish usually set the cycle, so name the temper, the specification and any later joining on the order.

CNC turned C36000 free-cutting brass parts with bright machined faces, threaded fittings, a knurled knob and small precise pins.

A 12 mm (0.47 in.) brass bar turned at the speed a carbide table recommends for the best free-cutting brass, 800 m/min (2,625 ft/min) at a chip thickness of 0.8 mm, would need the spindle at about 21,200 rpm, and the monograph that publishes the figure warns that maximum spindle speed often puts its values out of reach. That gap between what the alloy allows and what the machine can give is the first fact of machining C36000: the material is rarely the limit, and the part, the spindle and the chip are.

What Makes C36000 the Reference Brass for Turned Parts

C36000 is a leaded copper-zinc alloy built to be cut. The Copper Development Association’s data page gives its composition as 60.0 to 63.0 % copper, 2.5 to 3.0 % lead, iron at 0.35 % maximum and zinc as the remainder, with copper plus the named elements at 99.5 % minimum. The same page lists its machinability rating as 100, the top of the scale against which other copper alloys are ranked.

The scale itself is worth knowing. The German Copper Institute’s monograph i.18, “Recommended machining parameters for copper and copper alloys”, notes that its ratings are the CDA ratings measured by the ASTM E618 method, with CuZn36Pb3 as the American reference, and that Europe uses CuZn39Pb3 as its reference instead. Both references are assigned 100, and the index falls in steps of ten for alloys that cut less freely.

Lead does the work. The monograph explains that lead is practically insoluble in the copper-zinc matrix and, finely dispersed, acts as a chip breaker and sometimes as a friction-reducing lubricant. It adds that lead above 3.5 % is uncommon, because a fine dispersion becomes hard to achieve and the small gain in machinability does not justify the loss in mechanical properties.

Table 1. Properties of C36000 from the CDA data page and a brass mill’s product page, with the condition each figure belongs to.
Property Value, metric Value, US Condition and source
Density 8.50 g/cm³ 0.307 lb/in.³ at 20 °C (68 °F), CDA
Melting range, solidus to liquidus 888 to 899 °C 1,630 to 1,650 °F CDA
Electrical conductivity 26 % IACS 26 % IACS at 20 °C (68 °F), CDA
Thermal conductivity 116 W/m·K 67 Btu/ft·h·°F at 20 °C (68 °F), CDA
Coefficient of thermal expansion 20.5 × 10⁻⁶ /K 11.4 × 10⁻⁶ /°F 20 to 300 °C (68 to 572 °F), CDA
Specific heat 377 J/kg·K 0.09 Btu/lb·°F at 20 °C (68 °F), CDA
Modulus of elasticity in tension 96.5 GPa 14,000 ksi CDA
Modulus of rigidity 36.5 GPa 5,300 ksi CDA
Tensile strength, typical 386 MPa 56 ksi typical, Mueller Brass C36000 product page
Yield strength, typical 310 MPa 45 ksi typical, Mueller Brass C36000 product page
Elongation, typical 25 % 25 % typical, Mueller Brass C36000 product page
Hardness, typical 72 HRB 72 HRB typical, Mueller Brass C36000 product page
Machinability rating 100 100 CDA scale

The typical strengths in the table belong to one mill’s product. The CDA page splits its mechanical figures by form, temper (soft anneal O60, half hard H02, hard H04) and section size, and the minimum tensile strength of a half-hard bar changes with diameter. A drawing that depends on strength names the temper and the bar size rather than a single typical value.

C36000 is chosen for the chip, not for the strength. Its rating of 100 sets the scale, and its mechanical figures move with temper and bar diameter.

C36000 and the European Free-Cutting Brasses

A buyer converting a European drawing to an American bar, or the reverse, meets a cross-reference that is looser than it looks. The DKI monograph’s classification table pairs each EN designation with a UNS number, and none of its leaded brasses is paired with C36000.

Table 2. Leaded brasses near C36000, as paired and rated in the DKI monograph, with C36000 from the CDA page.
EN designation EN number UNS number given Tensile strength, MPa (ksi) Hardness, HB Tool geometry class Machinability rating
CuZn36Pb3 CW603N C35600 340 to 550 (49 to 80) 90 to 150 A 100
CuZn39Pb3 CW614N C38500 360 to 550 (52 to 80) 90 to 150 A 100
CuZn35Pb2 CW601N C34200 330 to 440 (48 to 64) 90 to 130 A 90
CuZn40Pb2 CW617N C37700 360 to 550 (52 to 80), shared cell 90 to 150, shared cell not stated 90
not listed by DKI not listed C36000 see Table 1 see Table 1 not stated 100 on the CDA page

The pattern is clear enough for purchasing. CuZn36Pb3 and CuZn39Pb3 sit at the same rating and geometry class as C36000, and the DKI text calls CuZn36Pb3 the American reference alloy. The table, however, names C35600 beside CW603N. A drawing that says “C36000 or equivalent” leaves the equivalence to the supplier, and the material certificate then decides what was bought.

US specifications for the alloy appear on the CDA page: ASTM B16/B16M for free-cutting brass rod, bar and shapes for screw machines, SAE J461 and J463, and AMS 4610 for half-hard free-cutting bars and rods. Mueller Brass’s product page lists ASTM B16, SAE J463 and AMS 4610 as equivalent specifications. ASTM’s own abstract of B16/B16M-24 describes rod, bar, wire and shapes of any cross section in UNS C36000 or C36010 for high-speed screw machining and moderate thread rolling, with requirements for chemistry, temper, tensile strength, Rockwell hardness and shape, and treats its SI and inch-pound values as separate standards that are not to be mixed.

Cutting Speeds for Turning, Drilling and Tapping Free-Cutting Brass

The DKI monograph keys every cutting table to the machinability rating, and its own procedure is to find the alloy’s rating and read the row. For a bar rated 100 the numbers are high.

Table 3. Recommended cutting data for copper alloys rated 100, from DKI monograph i.18, Tables 13 to 20.
Operation Tool Cutting speed, m/min (ft/min) Condition
Turning carbide 1,260 (4,134) chip thickness h 0.1 mm (0.004 in.)
Turning carbide 1,000 (3,281) h 0.32 mm (0.013 in.)
Turning carbide 800 (2,625) h 0.8 mm (0.031 in.)
Turning HSS 154 (505) h 0.1 mm (0.004 in.)
Turning HSS 85 (279) h 0.32 mm (0.013 in.)
Turning HSS 60 (197) h 0.63 mm (0.025 in.)
Drilling HSS 80 (262) feed by diameter, see text
Drilling solid carbide, 3 to 20 mm 250 (820) feed by diameter, see text
Drilling indexable carbide inserts 400 (1,312) larger holes
Tapping carbide N10 40 (131) none stated
Tapping HSS uncoated or coated 20 or 30 (66 or 98) none stated
Face milling uncoated carbide inserts 580 or 540 (1,903 or 1,772) hz 0.1 or 0.2 mm
Face milling polycrystalline diamond 1,050 or 1,000 (3,445 or 3,281) hz 0.1 or 0.2 mm
End milling HSS uncoated or coated 45 or 80 (148 or 262) peripheral milling
End milling solid carbide uncoated or coated 140 or 280 (459 or 919) peripheral milling

The Conditions Behind the Turning Row

The turning values rest on a tool life criterion. The monograph states them as valid in about 70 % of cases, for a flank wear land VB of about 0.6 mm at the end of life and a tool life of 30 to 60 minutes for carbide in group N10 or N20, or 45 to 90 minutes for HSS grade HS10-4-3-10.

Several corrections follow, and each changes the number a buyer sees quoted.

  • To double tool life, lower the speed by about 16 % for carbide and about 10 % for HSS.
  • If end of life is set at VB 0.4 mm instead of 0.6 mm, lower the speed by about 35 % for carbide and 15 % for HSS to keep the same life.
  • For form turning, grooving, parting off and threading, where chip flow is restricted, lower it by about 40 % for carbide and 50 % for HSS.
  • For HSS other than HS10-4-3-10, multiply by 0.82 for HS10-1-4-5, 0.76 for HS12-1-4, 0.72 for HS6-5-2 and 0.65 for HS2-9-1.

Drill Feeds by Diameter

Feed in drilling depends mostly on the drill diameter. Table 15 of the monograph gives, for HSS drills, 0.1 to 0.16 mm per revolution at 3 to 5 mm, rising through 0.25 to 0.32 mm at 8 to 12 mm to 0.4 to 0.5 mm at 16 to 20 mm. Carbide drills run finer feeds, from 0.08 to 0.12 mm at 3 to 5 mm up to 0.3 to 0.35 mm at 16 to 20 mm. Alloys that give short, broken chips take type H drills under DIN 1414, which match the monograph’s geometry class A.

Screw Machine Practice From a Bar Datasheet

Mueller Brass, a brass mill, gives the working ranges of a screw machine instead on its C36000 product page: 91 to 305 m/min (300 to 1,000 ft/min) and 0.05 to 0.38 mm (0.002 to 0.015 in.) per revolution for lathe tools, the same speeds with 0.08 to 0.51 mm (0.003 to 0.020 in.) per revolution for drills, 61 to 152 m/min (200 to 500 ft/min) for milling cutters, the lathe speeds with 0.03 to 0.08 mm (0.001 to 0.003 in.) per revolution for form tools, and 30 to 61 m/min (100 to 200 ft/min) for taps. The same page calls C36000 the industry standard for general machining and high-volume production, with machinability that permits full use of a screw machine’s capabilities.

The two documents disagree by a factor of three or more on turning speed, and both are right for their setting. The DKI turning row assumes carbide with a stated wear criterion; the mill’s page describes screw machine practice with lathe, drill, milling and form tools. The monograph itself warns that its speeds are often out of reach because of the maximum spindle speed or a very small workpiece diameter. For the 12 mm bar of the opening, 91 to 305 m/min means about 2,400 to 8,100 rpm.

On a small brass part, spindle speed and chip control set the cycle long before the alloy does. A quotation that assumes the table speed on a 6 mm diameter assumes a machine that may not exist in the shop.

Chip, Force and Finish on a Leaded Brass Bar

Free-cutting brass is light on the tool. The DKI monograph lists the principal value of specific cutting force kc1.1 for CuZn39Pb3 at 450 N/mm² with a gradient 1−mc of 0.68 in one data set and 389 N/mm² with 0.69 in another, against 820 N/mm² for the sulfur-bearing copper CuSP. The Copper Institute’s own machining page puts it more broadly: compared with steels of the same strength, the cutting forces and the chip volume removed per unit of time and power are many times more favorable for free-cutting brasses.

The chip that makes it easy also has a cost. Alloys with chip-breaking additions form fine, needle-like or discontinuous chips, and the monograph notes that this makes leaded alloys more prone to chatter marks than lead-free alloys of the same tensile strength. The monograph’s answer is a machine without play and tools and holders of sufficient rigidity.

Tool Geometry Class A

The monograph classifies CuZn39Pb3 as I.A.100: machinability group I, tool geometry class A, rating 100. Class A in its Table 12 means a rake angle of 0 to 8° with a 6° clearance for carbide, and 5 to 10° rake with 8° clearance for HSS, with a 50° back wall where a chip breaker is ground. Mueller’s page gives lathe tools 0 to 5° back rake and 6° clearance, drills 0° rake with 12 to 15° clearance, milling cutters 0 to 10° rake with 10 to 15° clearance, and form tools 0 to 5° rake with 7 to 12° clearance.

Both documents keep the rake low, at or near zero for the screw machine tools, and the drill rake at zero.

Finish as the Judging Criterion

For free-cutting alloys the achievable surface is the criterion that matters most. The monograph says so directly: turned parts in free-cutting brass often need decorative surfaces, which frequently means smoothing or precision finishing, so surface quality is treated as the most important machinability criterion for alloys such as CuZn39Pb3, CuZn40Pb2 and the leaded nickel silvers. Too much lead, it adds, also impairs polishability.

The Copper Institute names four criteria in all: tool wear, chip formation, cutting force and surface finish. In brass the first three are usually easy, and the fourth decides whether a part is accepted.

What the Datasheet Leaves Out for a Machined Brass Part

A machining datasheet answers how fast to cut and is silent on what happens after the part leaves the machine. Several lines from the opened documents fill part of that gap.

  1. Hot and cold work. Mueller’s page rates the alloy poor in its capacity to be hot worked and able to be moderately cold worked.
  2. Joining. The CDA page rates C36000 excellent for soldering, good for brazing and not recommended for most welding methods. The DKI monograph is more cautious about leaded alloys that are soldered or welded after machining, calling them of limited applicability.
  3. Lead content and regulation. Mueller notes that the alloy was recently amended to a lower maximum lead percentage, and the DKI monograph cites European Directive 2000/53/EC, which restricts heavy metals in vehicle components.
  4. Bar tolerance. Mueller lists rounds from 6.35 to 101.6 mm (0.250 to 4.000 in.) holding ±0.038 mm (±0.0015 in.) up to 12.7 mm (0.500 in.) and ±0.051 mm (±0.0020 in.) from 12.7 to 25.4 mm (0.500 to 1.000 in.), while hexagons are held to about twice those values, ±0.076 mm (±0.0030 in.) up to 12.7 mm.

The joining line deserves a decision before release. A part that will be soldered into an assembly is not the same purchase as a part that is only machined, and the order says which it is.

Thermal figures from the CDA page also matter at the inspection bench. With an expansion coefficient of 20.5 × 10⁻⁶ per kelvin, a 50 mm (1.97 in.) brass length grows by about 5 µm (0.0002 in.) for every 5 K of difference between the part and the gauge.

Choosing C36000 for a Turned Part

The alloy earns its place on parts that are mostly turning, drilling and threading, with modest loads and a visible surface. Its high rating means the cycle is set by the machine and the chip, and its low cutting force asks less of the setup than a steel of the same strength.

The buying decisions that follow are few and specific.

  • Name the alloy by its UNS number and the specification, for example C36000 to ASTM B16/B16M-24, and the temper.
  • If a European grade is acceptable, name it, such as CuZn39Pb3 (CW614N), instead of writing “or equivalent”.
  • State whether the part will be soldered, brazed or cold formed after machining.
  • State the surface wanted on visible faces, since finish is the criterion the alloy is judged by.
  • State any restriction on lead content that applies to the product.

For parts that start as a first batch of turned pieces and grow toward a steady run, a buyer can read about low-volume metal CNC and bridge production with the alloy, temper and finish already fixed on the drawing.

Sources and Further Reading

Request a Metal CNC Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Metal CNC chosen.

Request a Quote