AluminumInspection6061-T6

How Burrs Form on Machined Aluminum and How They Come Off

A burr is the last chip, so its size follows the alloy, the temper and the tool, and a signed edge size on the drawing turns it into a measurement.

CNC machined aluminum L-shaped brackets with drilled holes, one turned to show a fine burr ridge on a hole exit edge, and a hand deburring tool with a swivel blade and a plain metal handle.

The height gauge used in one aluminum drilling study reads to 0.0005 in (13 µm), and that is the resolution at which a burr gets measured at all. A burr taller than that gauge’s step is already a visible ridge on the exit side of a hole, and one only a few times taller can catch a thumb, lift a seal or break loose inside an assembly. Burr formation is a chip-formation problem that continues past the end of the cut, and the metal pushed over the edge is what remains of it.

On a drawing, the same edge is one line. In the cutting zone, it is the place where a tool stops supporting the material it is cutting, and what happens there depends on the alloy, the temper, the tool, the feed and the way the tool leaves the part. The sections below follow a burr from its formation to the edge callout that limits it and the finishing step that removes it, using a published review chapter on aluminum alloys and the text of the ISO standard for edges of undefined shape.

Why a Cutting Tool Leaves a Burr on Aluminum

A burr is a projection of material beyond the workpiece limits. Its opposite is a negative burr, a missing portion of the edge where material broke away instead of being pushed. The review chapter by Niknam, Zedan and Songmene treats both as products of plastic deformation: the metal is stretched past the elastic limit near an edge that has nothing behind it, and it flows or tears instead of shearing cleanly.

Ductility decides how far the flow goes. The chapter reports that more ductile materials tend to form larger burrs, and that the effect grows with cutting speed and feed in some of the cited work. A brittle material goes the other way and leaves fractured, negative burrs on the edge. Soft, gummy aluminum conditions sit at the ductile end, which is why aluminum has the reputation of cutting easily and finishing badly.

The shape of the edge matters as much as the alloy. Cutting tests cited in the chapter found that workpiece edge angles below 90° generate long, thin burrs, while edge angles of 90° or larger give short, thick ones. An external corner that is thin and sharp gives the tool nothing to push against.

A burr is the last part of the chip. It forms where the tool exits or enters the part, it grows with the ductility of the alloy, and it does not disappear by changing speed and feed alone.

Burr formation is almost impossible to avoid, according to the review, and one cited study found that feed rate, cutting speed and tool geometry changed it but never removed it. The aim on the shop floor is therefore a burr of known size and known place, small enough to remove in one planned step.

Primary and Secondary Burrs

The literature separates a primary burr from a secondary one. A secondary burr forms after the primary burr breaks, and it is smaller than the depth of cut, while the primary burr is larger. In face milling of aluminum, the review cites work showing that the secondary burr is dominated by depth of cut and feed rate. Raising the feed in milling made burrs smaller and produced secondary burrs that were easier to remove.

A part that leaves the machine with a thin secondary burr along an edge can look finished and still carry a ridge that a gloved finger finds at once. Inspection language that says “free of burrs” needs a size behind it, a point the standard section below returns to.

Burr Types and Where They Sit on a Machined Part

Four main types appear in the literature on machining burrs: the Poisson burr, the rollover burr, the tear burr and the cut-off burr. The Poisson burr is the sideways bulge of material. Engineering mechanics adds a distinction, noted in the chapter, since the Poisson effect strictly belongs to the elastic range, so some authors call it a side burr.

For a buyer, the location of a burr is more useful than its name. The same cutter makes different burrs at different places on the same feature, and each place has its own remedy.

Table 1. Where burrs form in drilling and milling, and what the review chapter reports about each
Location Operation What the review reports
Exit burr at a drilled hole Drilling Larger than the entrance burr and the hardest to remove, which is why most studies measure it
Entrance burr Drilling and milling Large entrance burrs appeared when worn tools were used, through a different tool engagement rather than back cutting
Exit up-milling side burr Slot milling Thickness controllable by feed per tooth, depth of cut and tool; height depends on interacting parameters
Exit bottom burr Slot milling Grows with a larger insert nose radius, while the side burr shrinks
Burr at a part edge in face milling Face milling Exit angle and tool geometry strongly change burr size and edge breakout in aluminum-silicon alloys

A drilled cross hole that breaks into a bore is the case that hurts most. The exit burr forms inside a passage the tool cannot reach again, and its removal needs a method that gets into the bore.

Burr Value and Why Height and Thickness Matter

The chapter describes a single “burr value” built from four measurements: root thickness, height, thickness and root radius. It then points out that all four are slow to measure and that the value does not help choose a deburring method. Of those parameters, burr height and thickness are the two used to judge how hard a burr is to remove.

A tall, thin burr lifts off easily and leaves a short stub. Short and thick, by contrast, is a burr that stays rooted in the parent metal and needs a tool that cuts it away.

Alloy, Temper and Cutting Data That Change Burr Size

Aluminum alloys do not burr alike. The chapter compares drilling of four alloys under the same conditions: 6061-T6, a higher-strength 6061 variant, 6262-T6 (6061 with 0.5 wt% lead and 0.4 wt% bismuth) and an alloy of the 4XXX family with 8 % silicon, all at tempers aged to T6. Ductility put the 4XXX alloy at the worst end, with a transient burr type and the tallest exit burrs of the group. Only uniform burrs came from the 6262-T6 and the higher-strength 6061, while 6061-T6 and the 4XXX alloy produced both uniform burrs and the transient or crown burrs that are generally difficult to remove.

The drilling tests ran at four cutting speeds from 91.44 m/min (300 sfm) to 274.32 m/min (900 sfm), with feed rates up to 0.175 mm/rev on the plotted axes. Burr height fell as speed rose, and in the drilling data lower feed gave a taller burr. The review reports a possible interaction between the two, which is why neither number alone predicts the result.

A Temper Study on Cast A356

The case study in the chapter shows how much heat treatment alone can move a burr. Blocks of cast A356 (Al-Si-Mg), 300 × 100 × 20 mm, were drilled dry with an uncoated high-speed-steel twist drill of 9.525 mm (3/8 in) diameter and 118° point angle, at 60, 180 and 300 m/min and 0.15 mm/rev. Five conditions were compared: as cast (T0), solution treated at 540 °C for 8 hours and quenched in 60 °C water (T4), and three artificial agings of 5 hours each at 155 °C (T61), 180 °C (T62) and 220 °C (T7). Each condition was repeated four times and the burr heights averaged.

Table 2. Temper and drilling burr height on A356, as ranked in the review chapter
Condition Treatment Hardness note Burr height ranking
T0 As cast Not stated Highest group
T4 540 °C for 8 h, quenched in 60 °C water Not stated Highest group
T61 T4, then 155 °C (311 °F) for 5 h Peak hardness, 85 to 90 HRE Lowest
T62 T4, then 180 °C (356 °F) for 5 h Near peak, then falling Higher than T61
T7 T4, then 220 °C (428 °F) for 5 h Falling with overaging Higher than T61

Peak-aged T61 gave the smallest burrs. Hardness is the explanation offered is that a harder matrix resists deformation in the shear zone, so the material holds its position and cuts instead of folding over, while the silicon particles in the alloy abrade the tool edge. That has a cost the chapter acknowledges: a low burr and high cutting force arrive together.

The temper a supplier receives is a deburring decision. Peak-aged material burrs least in this study, and the soft conditions burr most.

What the Tool and the Strategy Add

Tooling carries as much of the result as the alloy. Findings from the cited work, collected these findings from the cited work:

  • Sharp edges with positive rake avoid built-up edge, and so reduce burr size.
  • A drill diameter of 8 to 10 mm gave low burr height in one study.
  • Positive axial rake with negative radial rake gave acceptable burr size and surface in another.
  • Diamond end mills at high cutting speed were reported able to reach burr-free conditions.
  • Coating had a negligible effect on face-milling burrs.
  • Tool wear enlarges the contact between burr and tool, raises cutting force and increases burr size.

The strategy list in the same chapter is useful when a part has a known burr trouble spot. Tool path planning that chooses the machining direction and the tool engagement angle, backup materials at exit edges, adjusted cutting parameters and coolant all reduce burr size. The review also reports that chamfering external edges before the cutting operation is an excellent approach, because it removes the thin edge that would deform. Coolant is not a free choice, though, because the authors note that for certain materials a lubricant hardens burrs and complicates deburring.

How Burr Height Gets Measured

The case study recorded burr height with a mechanical height gauge of 0.0005 in (13 µm) sensitivity, and every condition was drilled four times so that an average could stand for the scatter. Two lessons carry over to an order. A burr height without its measuring method is a claim, and a single hole is not a sample of anything.

The chapter’s authors add that the burr formation mechanism depends highly on chip formation, so the cutting force is a signal. In the slot-milling studies it cites, exit burr thickness correlated with changes in the tangential cutting force. The review also reports that a worn tool enlarges burrs and raises cutting force, so the edge condition on the last part of a tool’s life is not the edge condition on the first.

Edge Callouts That Tell the Shop How Much Burr Is Allowed

A drawing draws the ideal shape with no deviation at the edges. ISO 13715:2017, titled Technical product documentation, Edges of undefined shape, Indication and dimensioning, gives the symbol for the edge the part actually needs. Its introduction says the conditions it covers include external edges free from burr or with a burr of limited size, and internal edges with a passing.

The standard uses two terms. An undercut is a deviation inside the ideal shape of an edge, bounded by two tangent straight lines to the adjacent features. A passing is a deviation outside that shape. The standard adds that a burr or a flash can be considered a special case of external passing.

Symbols and Size on the Drawing

Inside the basic graphical indication sits the symbol element, and the minimum indication is the type of undefined edge. After the sign comes the size.

Table 3. Symbol elements for undefined edges in ISO 13715:2017, clause 4.2 and 4.3
Element Meaning External edge Internal edge
+ (plus) Permitted excess material, a passing Passing (burr) permitted, undercut not permitted Passing permitted, undercut not permitted
− (minus) Required material removal, an undercut Undercut required, passing not permitted Undercut required, passing not permitted
± (plus or minus) Passing or undercut permitted Both permitted Both permitted, used only with a size

The size is the maximum deviation, placed after the symbol element. One positive limit sets the second limit at zero, so an undercut is not allowed. A negative value alone sets the second limit at zero and a passing is not allowed. Two limits are written one above the other, upper above lower.

The same document points to ISO 129-1 where a defined edge shape such as 1 × 45° is required. That boundary matters in practice: a chamfer drawn as a feature is a machined shape, and an edge callout is a tolerance on what the edge may do.

The 2017 edition deleted the earlier annex of recommended edge sizes and the definition of a sharp edge. A drawing note that says “break sharp edges” has therefore lost its standard-based meaning, and a number with a sign is what a shop can machine to and an inspector can measure to.

Deburring Methods and What Each Leaves Behind

Gillespie, cited in the chapter, counted 122 deburring and edge finishing processes in four families: mechanical, thermal, chemical and electrical. For machined aluminum the review concentrates on mechanical methods. Each trades speed against a side effect that the part carries onward.

  • Manual deburring. The most widely used method, for its flexibility and its lack of required technology. The review also reports that it brings wasted time, fatigue and inconsistent results when done dry by unqualified operators.
  • Bonded-abrasive deburring. Suited to heavy stock removal in manual or automated use. The review lists short tool life, dust, new burrs, effects on residual stress and surface quality, and no access to some sides of a part among its disadvantages.
  • Brush deburring. Fast and flexible, used on aluminum cylinder heads and shown on 6061-T6 in the chapter. Its side effects are new burrs, changes in part size, and effects on fatigue life and residual stress.
  • Deburring in the machining center. A brush or a cutter in the tool holder lets the machine deburr in the same setup, and a water jet nozzle can be traversed around an edge for reasonable but not complete removal.
  • Robotic deburring. Five-axis compliant tools remove most burrs but not all, according to the review.

Burrs that stay on parts cause trouble the review lists plainly: injuries to assembly workers, debris during operation, and burrs adhering to the part that loosen later and damage mating parts.

Every deburring step changes the part too. A brush that rounds an edge by a few tenths of a millimeter has altered a feature, and the edge callout above is what decides whether that is acceptable.

Questions to Settle Before the First Order

  1. Which edges carry a symbol and a size, and which fall under a general note?
  2. Is any hole an exit into a bore, where the burr cannot be reached afterward?
  3. Does a finish such as anodizing follow, so that an edge radius also has to hold a coating?
  4. Which method does the supplier plan for each edge, and does it add a burr or change a size?

The first article is the place to answer them on actual metal. A supplier that machines to a signed edge size, deburrs by a named method and measures the result on the first parts gives a buyer evidence rather than a statement that the edges are clean.

A drawn edge with a sign and a size, an alloy in the temper the part was designed around, and one named deburring step turn a burr from an argument into a measurement. Where that edge control is part of a first run, low-volume CNC machining carries the parts through the first lots, and the same edge callouts then carry over into bridge production.

Sources and Further Reading

Request a Metal CNC Quote

Send the 2D drawing and the 3D file, with the quantity and the stage of the project. An engineer replies within 1 working day.

The quote form, the mutual NDA and the private folder for your files are on Protolis Atelier, with Metal CNC chosen.

Request a Quote